Why Vibration-Welded Parts Fail Leak Tests

A vibration-welded part that fails a leak test usually has one of a small number of causes, and each leaves a different clue. The leak is rarely “the weld was bad” in general. It is a gap in one place, a cold section, a channel in the flash, or a crack that opened after welding. Find the leak path first, then fix its cause.

Start by locating the leak. Bubble-test the part under water, or use a tracer and a sniffer, and mark the exact spot. Then section that spot. The section tells you whether the joint never fused, fused and then cracked, or fused everywhere except at one feature. That distinction decides the fix.

Infrared heating mould and upper and lower cold moulds inside a vibration welding machine

Leak Failure Map: Where to Look First

Use this table before you touch a parameter. Match the symptom to the likely cause, confirm it by sectioning, then change one thing.

SymptomMost likely causeConfirm byFirst fix
Leak at one cornerUneven melt thereSection the cornerEven out contact and fixture support
Leak all around the jointCold weld; too little meltSection in several placesIncrease melt; check amplitude and time
Leak after a delayCrack from stress or coolingSection the crackCheck resin, drying, and cooling
Leak only on some partsPart variation or moistureCompare good and bad partsCheck dimensions, warpage, dryer logs
Leak at a port or channelInternal flash or a trapped channelBorescope the channelAdd a flash trap; limit collapse
Leak rate drifts over a runTool wear or driftPlot collapse and leak rateInspect tooling

Cause 1: The Joint Never Fused in One Place

A partial cold weld is the most common leak cause we see. The joint looks closed outside, but a section shows a line where the two faces never melted together. Air or fluid follows that line straight through.

Why does one area stay cold? Usually because contact was uneven. A warped part touches first on one side and melts there, while the rest never gets the same pressure. A rib can hold the halves apart, and a worn nest lets the part tilt.

The fix is mechanical before it is a parameter change. Check part flatness, seating, and tooling wear at the locating features. Only then adjust the process — to even out heating, not simply to add more energy. More time on an uneven joint often melts the hot side more and leaves the cold side cold.

Cause 2: Too Little Melt Overall

Sometimes the whole joint is under-melted. The section shows a thin, broken melt zone all around, or almost no melt at all. The part may pass a handling test and still fail a leak test, because a leak needs only a hairline path.

Under-melting usually comes from too little energy: amplitude too low, weld time too short, or pressure too low to keep the faces in contact. It can also come from a setting copied from a different part. The right point in the 100–240 Hz range depends on part size and stiffness.

On the Jfortune JFR-850, frequency is 210–250 Hz and amplitude is 0.6–1.8 mm, with a 7.1 kW servo motor driving the vibration head. Increase amplitude or time in small steps, section the joint, and stop when fusion is continuous. More energy past that point makes more flash, not a better seal.

Cause 3: The Joint Fused, Then Cracked

A leak that appears hours after welding, or after the part cools fully, often means the joint fused and then cracked. The crack may be tiny, but a leak test will find it.

Cracking has several drivers: residual stress from uneven cooling, clamping too hard during cooling, brittle resin from over-drying or degraded regrind, and moisture leaving pores that later open into a leak path.

Check the material first: resin grade, regrind share, and drying record against the supplier’s recommendation. Then look at cooling — is the part held under load, ejected hot and bent, or stacked while still warm?

Cause 4: Internal Flash and Trapped Channels

Internal flash is easy to miss, because the outside of the part looks clean. Melt squeezed into a fluid channel can leave a thin channel of its own, or a flap that lifts under pressure and opens a path.

This is a joint-design problem first. A flash trap — a groove or pocket beside the weld bead — gives melt a place to go before it reaches a channel or port. A collapse limit stops the parts closing further once the joint is formed.

If internal flash is suspected, borescope the channel or cut the part open. Do not rely on the outside appearance. For more on controlling where melt goes, see our flash-control guidance. The process is explained in how vibration welding works.

Cause 5: The Test Itself Is Misleading You

Not every leak-test failure is a weld failure. Before you rework the process, check the test.

Pressure-decay testing is sensitive to temperature. A part still warm from welding will show a pressure change as it cools, and that can look like a leak. Let parts reach a stable temperature before testing, and test a known-good part as a control.

Sealing matters too. A test fixture sealing on a warped face, a worn seal, or a port with flash on it will leak at the fixture, not at the weld. Mark the leak location: if it is always at the test seal, the weld may be innocent.

Test pressure matters as well. Testing far above working pressure can open a joint that would seal in service. Test at the pressure the specification calls for, and record temperature, hold time, and the pass limit with the result.

How Infrared Preheating Changes the Leak Picture

Infrared preheating helps leak performance because it evens out the start. In the JFR-850 10-step cycle, the infrared heater warms the upper and lower parts at the same time before vibration starts, so melt forms across the joint at once instead of in one hot spot first.

A Fix Workflow That Works

When leak failures appear, work in this order and do not skip steps.

Locate. Mark the exact leak spot with a bubble or tracer test. Do not guess from the test number alone.

Section. Cut through the leak spot and through a good area for comparison. Note whether the joint is cold, cracked, porous, or blocked by flash.

Compare parts. Measure failing parts against passing parts: flatness, dimensions, weight, and resin batch. A difference that tracks with failure is a lead.

Check material. Confirm grade, drying, and regrind. Moisture and degraded resin cause failures that look like process failures.

Change one thing. Adjust one parameter, or one tooling feature, then run at least five parts and leak-test them all. Record collapse, the section result, and the leak result together.

For the machine settings behind this workflow, see the servo vibration welding machine operation guide and infrared preheat vibration welding.

What to Send for a Leak Review

If you ask a supplier to help with a leak failure, send more than the leak rate. Send the drawings, resin grade and drying conditions, joint geometry, and the leak-test method with its pressure, temperature, and pass limit. Send photographs of the leak location and, if you can, a sectioned part.

Frequently Asked Questions

Why do parts pass a leak test at first, then fail later?

The joint may have fused and then cracked as it cooled, or under stress in assembly. Section the failed part, look for a brittle fracture or porous melt zone, and check resin and cooling before changing parameters.

Should I just weld longer to stop leaks?

No, not as a first step. Longer welding makes more melt and more flash, and can push melt into channels. First find where the leak is and whether the joint is cold, cracked, or blocked, then change the one variable that addresses that cause.

Can a leak test fail if the weld is actually good?

Yes. A warm part cooling during a pressure-decay test, a worn test seal, or a test pressure far above working pressure can all produce a false failure. Test at a stable temperature and check the fixture seal.

Does infrared preheating improve leak-tightness?

It can, because both surfaces are heated at the same time before vibration, so melt forms more evenly — especially at corners and ribs where leaks usually start. It helps a sound joint design; it does not fix a bad joint or wet resin.

How many parts should I test after a fix?

Test at least five parts after any change, and section at least one. A single passing part proves very little. Five passing parts with a continuous sectioned joint, plus a stable collapse reading, is a reasonable basis to resume production.

Get an Engineering Review

If vibration-welded parts are failing leak tests, send Jfortune your part drawings, resin grades, weld geometry, leak or strength requirements, and target cycle time. Include the leak-test method, the leak location, and a sectioned part if you have one.

Leave a Comment

Your email address will not be published. Required fields are marked *

Scroll to Top